CR729 Very reddish brown, semi matt
with darker spots
| Rather thick or it will be no spots. 1260-1280oC with one hour at the top temperature. One of the most red glazes I know based on ferric oxide in oxidation. You can try other simple boric frits with not too low maturing temperature instead of G-3. |
|
feldspar NGP | 37,22 | |
| bone ash | 12,41 | ||
| talc | 8,68 | ||
| petalite | 12,41 | ||
| quartz (flint) | 9,93 | ||
| ball clay | 7,44 | ||
| red ferric oxide | 6,95 | ||
| borax frit MOK G-3 | 4,96 |