92187 Fat greenish gray Celadon
A fat Celadon at its best when thick. No crackle. 1260-1280
o
C in normal to heavy reduction. Semi matt. White and colored stoneware clays.
potash feldspar NR
38,10
china clay
7,90
quartz (flint)
28,60
whiting
15,90
talc
9,50
red ferric oxide
1,10