| Always a good and
safe clear red, even in the least reduced parts of the kiln. Too thick it will run. 1260oC
with 1/2 hour oxidation at top temperature. Crackle on some clays. |
|
|
| nepheline syenite |
37,80 |
| quarts (flint) |
27,60 |
| borax frit MOK1 |
18,40 |
| ochre |
0,50 |
| whiting |
7,50 |
| dolomite |
7,50 |
| tin oxide |
0,75 |
| black copper oxide |
0,28 |
|