It is a pleasant semi
matt rose glaze with a good crackle pattern. 1270oC with half an hour of
oxidation at top temperature. Not too thick or thin. Works sometimes well on top of a
Peachbloom in a second firing. Then it can give very sharp dark red spots. |
|
|
nepheline syenite |
36,70 |
barium carbonate |
6,40 |
quartz (flint) |
27,50 |
zinc oxide |
3,70 |
whiting |
22,10 |
tin oxide |
3,70 |
copper carbonate |
1,10 |
|