It can be a very
pleasant semi glossy red glaze with strikingly darker spots. But not always! 1260oC
with half an hour of oxidation at top temperature. Not too thick or it will be a dull
redbrown. |
|
|
potash feldspar NR |
35,40 |
petalite |
5,20 |
quartz (flint) |
26,40 |
china clay |
1,70 |
borax frit MOK-G3 |
17,10 |
whiting |
13,10 |
tin oxide |
1,10 |
copper carbonate |
0,53 |
|