One of my most
popular crystal glazes based on zinc and lithium. Too thick it will run a lot, but it can
be controlled very exactly after a few tests. Always spray the glaze thinner near the
bottom of the pot. 1260oC with 1/2 to one hour at the top temperature. Does not
need a slow cooling. You can also try other combinations of coloring oxides. |
|
|
potash feldspar NR |
27,60 |
quarts (flint) |
32,20 |
dolomite |
3,48 |
zinc oxide |
18,70 |
barium carbonate |
4,44 |
china clay |
2,75 |
lithium carbonate |
6,82 |
rutile |
4,01 |
cobalt oxide |
1,06 |
|