| A glaze with zinc. You must
not apply it too thick. 1260-1280oC
with one hour at the top temperature. Does not
need a slow cooling. Small or no crystals. |
| |
|
| potash feldspar NR |
65,90 |
| dolomite |
16,15 |
| zinc oxide |
17,95 |
| red ferric oxide |
5,00 |
| cobalt oxide |
2,00 |
|