| A very popular crystal
glaze with zinc. You must not apply it too thick,
or it will be yellow gray and not so good.
1260-1280oC with one hour at the top
temperature. Does not need a slow cooling. You
can also try other combinations of coloring
oxides. Very small bright crystals. |
| |
|
| potash feldspar NR |
63,49 |
| dolomite |
15,87 |
| zinc oxide |
17,46 |
| rutile |
3,17 |
| cobalt carbonate |
1,59 |
|