| A semi glossy crystal
glaze based on frits and zinc. It tends to run not too much, but spray it thinner near the
bottom of the pot. 1260oC with ¾ hour at top temperature. Usually it behaves
very good. The crystals can be very complex and large. Use it alone or together with one
of my 6713-glazes. If you reburn it the crystals will be smaller. |
| boric frit MOK1 |
17,50 |
| zinc barium frit 90420 |
26,40 |
| quarts (flint) |
23,10 |
| zinc oxide |
22,10 |
| china clay |
4,30 |
| bentonite |
3,30 |
| rutile |
3,30 |
| cobalt carbonate |
1,30 |
| manganese carbonate |
2,00 |
|