| A semi glossy crystal glaze
based on frits and zinc. It tends to run not too
much, if not sprayed too thick. 1260oC
with ¾ hour at top temperature. Usually it
behaves very good. The crystals can be large. |
| |
|
| boric frit MOK1 |
17,60 |
| zinc barium frit 90420 |
26,40 |
| quarts |
22,20 |
| zinc oxide |
22,00 |
| china clay |
4,50 |
| bentonite |
3,30 |
| rutile |
4,00 |
| ferric oxide |
0,80 |
|