This glaze use to be very
safe. It is a green semi matt glaze with more or
less bright yellow crystals. 1270oC
with one hour at top temperature. Not too thick. |
|
|
nepheline syenite |
66,05 |
zinc oxide |
4,82 |
dolomite |
4,51 |
whiting |
4,82 |
ball clay |
4,51 |
quarts |
6,91 |
rutile |
8,41 |
copper oxide |
0,30 |
cobalt oxide |
2,00 |
red ferric oxide |
0,60 |
|