S422 Semi matt golden yellow
Very intensive golden yellow. More red when thin, glossier when thicker. 1270
o
C with one hour at top temperature. Safe glaze.
potash feldspar NR
64,35
whiting
18,93
china clay
3,15
Albany slip
5,68
rutile
7,89
red ferric oxide
6,31