A very pleasant smooth
glaze with a fine dark crackle pattern. Sometimes
very beautiful orange spots. If too thick it will
be glossy and not nice at all. Works best on
porcelain. |
|
|
nepheline syenite |
55,00 |
dolomite |
23,00 |
china clay |
21,00 |
quarts |
1,25 |
copper carbonate |
0,75 |
|