92099 Blue semi matt to glossy
Matt and best if fairly thin, glossy if too thick. 1260-1280
o
C in normal reduction.
potash feldspar NR
39,60
china clay
18,80
quartz
14,60
whiting
22,90
titanium oxide
4,20
cobalt carbonate
1,60