SH6 Shino glaze.
Use only on brown stoneware clays with or without lava or pyrite. Do not work on white or gray clays. Apply normal to thick. 1260-1280
o
C with good to heavy reduction.
nepheline syenite
33,33
ball clay
33,33
wollastonite
33,33