| Good black Tenmoku with
brown edges on white or light gray clay. Not too
thick. 1260-1280oC in normal
reduction. Semi glossy. More rost-colored with
yellow or brown bodies. |
| |
|
| Cornish stone |
64,57 |
| china clay |
9,71 |
| quartz |
12,91 |
| whiting |
16,12 |
| red ferric oxide |
8,06 |
|