5k5v Mushroom-colored silky matt
A good glaze based on zinc and barium. Very smooth. Not too thick. 1260-1280
o
C with 1/2 to one hour at the top temperature.
potash feldspar NR
44,67
whiting
4,67
zinc oxide
15,79
barium carbonate
16,26
china clay
13,93
rutile
4,67